AlNiCo Magnet
Isalibay ang AlNiCo Magnet Physical Properties | |||||||||
Materyal nga | Grado | Remanence | Si Rev. Temp.-Coeff. Ni Br | Pagpamugos | Si Rev. Temp.-Coeff. Sa Hcj | Max. Produkto sa Enerhiya | Max. Operating Temperatura | Densidad | |
Br (KGs) | Hcb (IKAW) | (BH) max. (MGOe) | g/cm³ | ||||||
Isotropiko | LN9 | 6.8 | -0.03 | 0.38 | -0.02 | 1.13 | 450 ℃ | 6.9 | |
Isotropiko | LN10 | 6.0 | -0.03 | 0.50 | -0.02 | 1.20 | 450 ℃ | 6.9 | |
Isotropiko | LNG12 | 7.2 | -0.03 | 0.50 | +0.02 | 1.55 | 450 ℃ | 7.0 | |
Isotropiko | LNG13 | 7.0 | -0.03 | 0.60 | +0.02 | 1.60 | 450 ℃ | 7.0 | |
Isotropiko | LNGT18 | 5.8 | -0.025 | 1.25 | +0.02 | 2.20 | 550 ℃ | 7.3 | |
Anisotropic | LNG37 | 12.0 | -0.02 | 0.60 | +0.02 | 1.65 | 525 ℃ | 7.3 | |
Anisotropic | LNG40 | 12.5 | -0.02 | 0.60 | +0.02 | 5.00 | 525 ℃ | 7.3 | |
Anisotropic | LNG44 | 12.5 | -0.02 | 0.65 | +0.02 | 5.50 | 525 ℃ | 7.3 | |
Anisotropic | LNG52 | 13.0 | -0.02 | 0.70 | +0.02 | 6.50 | 525 ℃ | 7.3 | |
Anisotropic | LNG60 | 13.5 | -0.02 | 0.74 | +0.02 | 7.50 | 525 ℃ | 7.3 | |
Anisotropic | LNGT28 | 10.8 | -0.02 | 0.72 | +0.03 | 3.50 | 525 ℃ | 7.3 | |
Anisotropic | LNGT36J | 7.0 | -0.025 | 1.75 | +0.02 | 4.50 | 550 ℃ | 7.3 | |
Anisotropic | LNGT32 | 8.0 | -0.025 | 1.25 | +0.02 | 4.00 | 550 ℃ | 7.3 | |
Anisotropic | LNGT40 | 8.0 | -0.025 | 1.38 | +0.02 | 5.00 | 550 ℃ | 7.3 | |
Anisotropic | LNGT60 | 9.0 | -0.025 | 1.38 | +0.02 | 7.50 | 550 ℃ | 7.3 | |
Anisotropic | LNGT72 | 10.5 | -0.025 | 1.40 | +0.02 | 9.00 | 550 ℃ | 7.3 | |
Sintered AlNiCo Magnet Physical Properties | |||||||||
Materyal nga | Grado | Remanence | Si Rev. Temp.-Coeff. Ni Br | Pagpamugos | Pagpamugos | Si Rev. Temp.-Coeff. Sa Hcj | Max. Produkto sa Enerhiya | Max. Operating Temperatura | Densidad |
Br (KGs) | Hcb (KA/m) | Hcj (KA/m) | (BH) max. (KJ/m³) | g/cm³ | |||||
Isotropiko | SALNICO4/1 | 8.7-8.9 | -0.02 | 9-11 | 10-12 | -0.03~0.03 | 3.2-4.8 | 750 ℃ | 6.8 |
Isotropiko | SALNICO8/5 | 5.3-6.2 | -0.02 | 45-50 | 47-52 | -0.03~0.03 | 8.5-9.5 | 750 ℃ | 6.8 |
Isotropiko | SALNICO10/5 | 6.3-7.0 | -0.02 | 48-56 | 50-58 | -0.03~0.03 | 9.5-11.0 | 780 ℃ | 6.8 |
Isotropiko | SALNICO12/5 | 7.0-7.5 | -0.02 | 50-56 | 53-58 | -0.03~0.03 | 11.0-13.0 | 800 ℃ | 7 |
Isotropiko | SALNICO14/5 | 7.3-8.0 | -0.02 | 47-50 | 50-53 | -0.03~0.03 | 13.0-15.0 | 790 ℃ | 7.1 |
Isotropiko | SALNICO 14/6 | 6.2-8.1 | -0.02 | 56-64 | 58-66 | -0.03~0.03 | 14.0-16.0 | 790 ℃ | 7.1 |
Isotropiko | SALNICO14/8 | 5.5-6.1 | -0.01 | 75-88 | 80-92 | -0.03~0.03 | 14.0-16.0 | 850 ℃ | 7.1 |
Isotropiko | SALNICO18/10 | 5.7-6.2 | -0.01 | 92-100 | 99-107 | -0.03~0.03 | 16.0-19.0 | 860 ℃ | 7.2 |
Anisotropic | SALNICO35/5 | 11-12 | -0.02 | 48-52 | 50-54 | -0.03~0.03 | 35.0-39.0 | 850 ℃ | 7.2 |
Anisotropic | SALNICO29/6 | 9.7-10.9 | -0.02 | 58-64 | 60-66 | -0.03~0.03 | 29.0-33.0 | 860 ℃ | 7.2 |
Anisotropic | SALNICO32/10 | 7.7-8.7 | -0.01 | 90-104 | 94-109 | -0.03~0.03 | 33.0-38.0 | 860 ℃ | 7.2 |
Anisotropic | SALNICO33/11 | 7.0-8.0 | -0.01 | 107-115 | 111-119 | -0.03~0.03 | 33.0-38.0 | 860 ℃ | 7.2 |
Anisotropic | SALNICO39/12 | 8.3-9.0 | -0.01 | 115-123 | 119-127 | -0.03~0.03 | 39.0-43.0 | 860 ℃ | 7.25 |
Anisotropic | SALNICO44/12 | 9.0-9.5 | -0.01 | 119-127 | 124-132 | -0.03~0.03 | 44.0-48.0 | 860 ℃ | 7.25 |
Anisotropic | SALNICO37/15 | 7.0-8.0 | -0.1 | 143-151 | 150-158 | -0.03~0.03 | 37.0-41.0 | 870 ℃ | 7.2 |
Mubo nga sulat: · Nagpabilin kami nga parehas sa taas gawas kung gipiho gikan sa kustomer. Ang temperatura sa Curie ug ang koepisyent sa temperatura alang lamang sa pakisayran, dili ingon usa ka sukaranan sa desisyon. · Ang labing taas nga temperatura sa pagtrabaho sa magnet mausab tungod sa ratio sa gitas-on ug diametro ug mga hinungdan sa palibot. |
Feature:
1. Ang AlNiCo magnet adunay taas nga remanent induction apan ubos nga coercivity. Naglihok kini nga lig-on sa grabeng temperatura, nga nagmintinar sa iyang magnetic nga mga kinaiya tali sa
–250ºC ug 550ºC. Pinasukad sa superyor nga magnetic induction, kadaghanan gigamit sa pagsukod sa mga kagamitan ug mga sistema sa pagtuki.
2. Ang Alnico usa ka mahuyang nga materyal ug mahimo lamang nga usbon sa panahon sa proseso sa paghulma. Ang orientasyon niini nakab-ot sa panahon sa pagtambal sa kainit, nga nagpatunghag magnetic field
uban ang gitakda nga direksyon sa magnetization.
3. Tungod sa ubos nga pwersa sa pagpugos, ang AlNiCo magnets dali nga maapektuhan sa reverse magnetic force ug epekto sa puthaw. Mao nga dali ra silang ma-demagnetize
pinaagi sa mga impluwensya sa gawas. Tungod niini nga hinungdan, ang mga magnet nga AlNiCo kinahanglan dili tipigan ug iputos sa parehas nga mga poste nga magkaatbang sa usag usa.
4. Sa open circuit, ang rasyon sa gitas-on/diametro (L/D) kinahanglang labing menos 4:1. Uban sa mas mubo nga gitas-on
5. Ang mga magnet nga AlNiCo maayo nga molihok batok sa oksihenasyon. Walay sapaw nga gikinahanglan alang sa nawong sa pagpanalipod.
Aplikasyon:
Paggamit sa taas nga pagkasensitibo nga mga produkto sama sa Mga Instrumento, Meter, Mobile Phones, Mga piyesa sa awto. Electroacoustic device, Motors, Pagtudlo ug Aerospace
militar, ug uban pa.
Ang tanan nga gipahayag nga mga kantidad gitino gamit ang standard nga mga sample sumala sa IEC 60404-5. Ang mosunod nga mga espesipiko nagsilbing reference value ug mahimong magkalahi.